Gas Metal Arc and Flux-Cored Arc Welding (GMAW/FCAW · Processes 131, 135, 136 and 138): Transfer, Gases, Pulsed Arc, Consumables and Quality

EXCELLENCE INDUSTRIAL TECH • ARTICLE IT-003 • BLOCK 1 OF 3

Gas Metal Arc and Flux-Cored Arc Welding (GMAW/FCAW · Processes 131, 135, 136 and 138)

Equipment, ISO 14175 gases, AWS and ISO wire classification, transfer modes, pulsed arc, calculations, quality, safety and the developments of 2023 to 2026.

GMAW is the most widely used arc process in manufacturing and the most robotized in the world. Its productivity comes from the continuous wire; its quality depends on understanding how wire feed speed, voltage, gas, contact-tip-to-work distance and waveform interact.

In gas metal arc welding (GMAW), known in Europe and Latin America as MIG/MAG, a consumable wire is fed continuously through a gun while a shielding gas surrounds the arc and the weld pool. MIG (metal inert gas) refers to inert gases, used mainly for aluminum, copper and other non-ferrous alloys; MAG (metal active gas) refers to mixtures with CO₂ or O₂, essential for welding steels. Tubular wires (FCAW/MCAW) use the same equipment.

It is found in vehicles, battery trays, structures, railcars, wind towers and ships. This article uses the most widely adopted ISO, IEC and AWS standards and records recent changes that affect procedures in force, such as the withdrawal of AWS A5.36 and AWS D1.1:2025.

Learning objectives

The student should be able to identify ISO 4063 processes 131, 132, 133, 135, 136, 138 and 114; explain arc self-regulation with a constant-voltage power source; select drive rolls, liner and contact tip; interpret ISO 14175 gas designations and AWS and ISO wire designations; distinguish short-circuit, globular, spray, pulsed and controlled short-circuit transfer; calculate conventional load voltage, deposition rate, arc time, gas consumption and heat input from instantaneous power; troubleshoot feeding problems and imperfections; apply qualification requirements; and recognize current and emerging technologies such as AI-based adaptive control, collaborative robotics under ISO 10218:2025 and wire arc additive manufacturing.

1. Process principle and ISO 4063 numbers

The arc is established between the wire, which is the electrode, and the workpiece. The gas — or the core flux, in tubular wires — protects the molten metal from atmospheric oxygen and nitrogen. ISO 4063, whose 5th edition was published in 2023 (replacing the 2009 edition and adding processes for plastics, without changing the numbering of arc processes), identifies each variant by a number used in WPSs and certificates.

ISO 4063 No.ProcessUsual AWS nameShielding
131MIG with solid wireGMAWinert gas (Ar, He)
132MIG with flux-cored wireFCAW-Ginert gas
133MIG with metal-cored wireGMAW-C / MCAWinert gas
135MAG with solid wireGMAWactive gas (CO₂, Ar+CO₂, Ar+O₂)
136MAG with flux-cored wireFCAW-Gactive gas
138MAG with metal-cored wireGMAW-C / MCAWactive gas
114Self-shielded flux-cored wireFCAW-Score flux, no external gas

1.1 Constant-voltage source and self-regulation

Conventional GMAW uses a constant-voltage power source (flat characteristic). The welder sets wire feed speed and voltage; current is the result. If the gun moves away and the arc lengthens, arc voltage rises slightly and current drops sharply, because the curve is flat; with less current, the wire melts more slowly, advances and restores the arc length. If the gun moves closer, the opposite occurs. This arc self-regulation allows welding at constant wire feed speed. In pulsed modes, electronic sources control current during part of the cycle, but the balance between feeding and melting still applies.

2. Equipment

MIG/MAG (GMAW) system components Power source constant voltage (flat curve) Wire feeder and drive rolls + (DCEP) shielding gas gun cable: wire, current and gas gun nozzle and tip return (work clamp) Teaching diagram. Water-cooled guns also include a coolant circuit.
Figure 1 — GMAW system components. Drive rolls, liner and contact tip must match the wire material and diameter.

2.1 Power source

Power sources may be transformer-rectifiers or inverters, which are lighter and faster. Synergic sources store curves by material, diameter and gas: when wire feed speed changes, the source automatically adjusts voltage and, in pulsed mode, the pulse parameters. IEC 60974-1 defines the duty cycle over 10-minute periods at 40 °C ambient and the conventional load voltage used for testing: for GMAW and flux-cored welding, U₂ = 14 + 0.05 × I₂. IEC 60974-14 covers calibration of these values.

2.2 Wire feeder

The feeder has a motor, gearbox, drive rolls and pressure adjustment. The groove profile depends on the wire: V-groove for solid steel wires, U-groove for aluminum and soft alloys, which deform easily, and knurled for tubular wires, which need traction without crushing. Four-roll drives are preferred for tubular wires and long cables.

2.3 Gun, liner, contact tip and nozzle

A coiled steel liner is used for steel; for aluminum, a PTFE or graphite liner reduces friction and avoids shaving the wire. The contact tip transfers current to the wire and is a wear item: an oval bore, loose thread or stuck spatter causes an unstable arc. The nozzle and diffuser deliver the gas. Manufacturers state, according to IEC 60974-7, the gun current rating for a duty cycle and gas type: the rating with argon-rich mixtures is lower than with CO₂.

2.4 Gas supply

Gas comes from cylinders, bundles or cryogenic tanks with a distribution line. The regulator reduces pressure, and the flowmeter shows the flow in L/min. Leaking hoses and fittings cause intermittent porosity. In automated lines, flow sensors record consumption and alarm on gas loss.

3. Shielding gases (ISO 14175 and AWS A5.32)

The gas protects the weld pool and also determines stability, transfer mode, penetration, spatter and part of the deposit chemistry. ISO 14175 classifies gases and mixtures by reactivity into groups and subgroups, and AWS A5.32M/A5.32:2021 adopts the same system as a modified adoption of ISO 14175:2008. The full designation gives group, components and contents — for example, ISO 14175 – M20 – ArC – 8 is argon with 8% CO₂.

ISO 14175 symbolComposition (volume)Behavior and typical use
I1Argon 100%MIG of aluminum, copper, nickel and titanium; GTAW
I3Argon + helium (0.5 to 95% He)Thick aluminum and copper: more heat, more fluid pool
M12Ar + 0.5 to 5% CO₂Stainless steels, spray and pulsed transfer
M13Ar + 0.5 to 3% O₂Stainless and carbon steel in spray
M14Ar + 0.5 to 5% CO₂ + 0.5 to 3% O₂Stainless and low-alloy steels
M20Ar + over 5 up to 15% CO₂Carbon steel in pulsed and spray, thin sheet, low spatter
M21Ar + over 15 up to 25% CO₂General-purpose carbon steel; flux-cored wires
M24Ar + 5 to 15% CO₂ + 0.5 to 3% O₂Carbon steel, high-productivity ternary mixtures
C1CO₂ 100%Carbon steel and tubular wires: deep penetration, no axial spray, more spatter

In practice: pure argon on carbon steel produces an erratic arc and irregular bead, because steel needs a small fraction of active gas; above about 15 to 20% CO₂, axial spray transfer is no longer obtained; CO₂ and O₂ oxidize part of the wire manganese and silicon, which is why GMAW wires contain deoxidizers; and helium adds heat, useful on thick aluminum and copper. Typical flow is 12 to 20 L/min, depending on nozzle, current and environment; excessive flow creates turbulence and draws in air.

Brazilian practice: gases are often sold under the supplier trade name. In purchase specifications and WPSs, the technical reference should be the ISO 14175 (or AWS A5.32) designation, not the brand, so that the mixture can be replaced by an equivalent one.

4. Wire classification: AWS × ISO × Brazilian practice

Carbon steel wires are classified in the United States by AWS A5.18/A5.18M (solid and metal-cored wires; 2023 edition) and AWS A5.20/A5.20M (flux-cored wires; 2021 edition). In the ISO system, ISO 14341 covers solid wires and ISO 17632 covers tubular wires for non-alloy and fine-grain steels. Both have system A (yield strength and 47 J) and system B (tensile strength and 27 J).

Reading wire designations: AWS × ISO AWS A5.18 solid wire ER electrode or rod 70 70 ksi tensile S solid -6 chemistry Mn and Si ISO 14341-A solid wire G solid wire 42 Re ≥ 420 MPa 4 47 J at −40 °C M21 test gas 3Si1 chemistry AWS A5.20 tubular E electrode 7 70 ksi tensile 1 all positions T tubular -1 usability type M mixed gas ISO 17632-A tubular T tubular 46 Re ≥ 460 MPa 4 47 J at −40 °C P rutile fast M21 test gas 1 all positions H5 H ≤ 5 mL/100 g Reading examples. Full requirements are in the standards; equivalence applies only to the certified product.
Figure 2 — Reading the most common designations. The same product family appears with different codes in each system; equivalence applies only to a product certified to both standards.

4.1 Solid wires

ER70S-6 is the most widely used carbon steel wire in the world: “ER” means electrode or rod, “70” means 70 ksi (≈ 480 MPa) minimum tensile strength, “S” means solid wire and “6” identifies the chemistry, with higher manganese and silicon that deoxidize the pool and tolerate light mill scale. Under ISO 14341-A, an equivalent product may appear as G 42 4 M21 3Si1: “G” for gas-shielded solid wire, “42” for 420 MPa minimum yield strength, “4” for 47 J at −40 °C, “M21” for the test gas and “3Si1” for the chemistry.

4.2 Flux-cored and metal-cored wires

  • Gas-shielded flux-cored (136): the slag supports the pool and allows out-of-position welding with high deposition.
  • Self-shielded flux-cored (114): the flux provides shielding; no cylinder is needed and it tolerates wind, ideal for field work. Some types run on DCEN.
  • Metal-cored (138): metal powder core, little slag, high deposition and good sidewall fusion; it behaves like a higher-yield solid wire.

Under AWS A5.20, E71T-1M means electrode (E), 70 ksi tensile (7), all positions (1), tubular (T), usability type 1 (rutile slag, DCEP) and testing with argon-CO₂ mixture (M); with pure CO₂ the suffix is C. Under ISO 17632-A, a fast-freezing rutile wire may be designated T 46 4 P M21 1 H5: tubular (T), 460 MPa minimum yield (46), 47 J at −40 °C (4), fast-freezing rutile core (P), M21 gas, all positions (1) and up to 5 mL of diffusible hydrogen per 100 g of deposited metal (H5). Carbon steel metal-cored wires remain in A5.18, as E70C-6M.

Standards update: AWS A5.36/A5.36M, which had created an “open” classification system for flux-cored and metal-cored wires (for example, E71T1-M21A2-CS1-H8), was withdrawn by AWS in 2023. AWS D1.1/D1.1M:2025 replaced its references with A5.18, A5.20, A5.28 and A5.29. Older catalogs still show A5.36 designations, and Canada decided to keep it; when revising a WPS to D1.1:2025, check the specification cited.

4.3 Other families and the situation in Brazil

FamilyISOAWS
Carbon steel — solid and metal-coredISO 14341A5.18
Carbon steel — flux-coredISO 17632A5.20
Low-alloy steels — solid / tubularISO 16834, ISO 21952 / ISO 17634, ISO 18276A5.28 / A5.29
Stainless steels — solid / tubularISO 14343 / ISO 17633A5.9 / A5.22
Aluminum and alloysISO 18273A5.10
Shielding gasesISO 14175A5.32

In Brazil, catalogs and WPSs mostly use the AWS designation, increasingly alongside the ISO designation. When purchasing, request the batch certificate (for example, type 3.1 under ISO 10474 or EN 10204, as per contract) and check that the classification printed on the package matches the WPS: changing ER70S-6 to ER70S-3 may require a procedure revision.

Block 1 summary

In GMAW with a constant-voltage source, wire feed speed sets the current and self-regulation maintains the arc length. Drive rolls, liner and tip must match the wire. The gas, identified by ISO 14175 or AWS A5.32, is a metallurgical variable. Solid and tubular wires carry different AWS and ISO designations for similar products, and the 2023 withdrawal of AWS A5.36 changed the references required by D1.1:2025.

Original technical diagrams produced for educational purposes. Classifications and requirements must be confirmed in the current editions of the standards and in manufacturers’ data sheets.

EXCELLENCE INDUSTRIAL TECH • ARTICLE IT-003 • BLOCK 2 OF 3

Metal Transfer, Parameters, Calculations and Qualification

Short-circuit, globular, spray, pulsed and controlled short-circuit transfer; inductance; wire feed speed, voltage and CTWD; worked calculations; welding technique; WPS and qualification.

5. Metal transfer modes

The way metal passes from the wire to the pool determines heat, positions, spatter and the risk of lack of fusion. It depends on current, voltage, diameter, material, gas and, in controlled modes, the waveform.

Teaching map of metal transfer modes current (wire feed speed) voltage short circuit globular spray Ar ≥ ~80% transition current pulsed: background ↔ peak No axial spray with pure CO₂. Conceptual boundaries: they depend on gas, diameter, material and power source.
Figure 3 — Teaching map of transfer modes. The pulsed arc alternates between background and peak, crossing the globular region without staying in it.

5.1 Short circuit

At low current and voltage, the droplet touches the pool before detaching, forming a metal bridge. Current rises, the bridge breaks by electromagnetic pinch and the arc reignites, up to about two hundred times per second. With low heat input and a small pool, it suits all positions and thin sheet. Its limitation is low energy: on thick sections there is a risk of lack of fusion (cold lap), often invisible on the surface. For this reason AWS D1.1 does not include short-circuit transfer (GMAW-S) among prequalified processes; for sheet steel, AWS D1.3 covers specific procedures.

5.2 Globular

At intermediate currents, or with pure CO₂, droplets larger than the wire diameter form, detach irregularly and are repelled from the arc axis. The result is spatter, irregular beads and limitation to the flat and horizontal positions. With solid wire in an argon-rich mixture, it usually indicates parameters between ranges.

5.3 Spray

Above the transition current, and with argon-rich mixtures, metal transfers as fine droplets aligned with the wire axis. The arc is stable, almost spatter-free and with high deposition. The transition current increases with diameter and varies with gas: manufacturer tables give typical values of about 220 A (steel, 1.1 mm, Ar + 2% O₂) and 275 A (1.6 mm). The large pool restricts spray on steel to the flat and horizontal positions.

5.4 Pulsed arc (GMAW-P)

In the pulsed arc, the source alternates between a background current, which keeps the arc alive with little heat, and a peak current, above transition, which detaches one droplet per pulse. Spray-type transfer is obtained at low average current, in all positions and with less spatter and heat. It is the preferred mode for aluminum, stainless steels and medium thicknesses. AWS D1.1:2025 now addresses GMAW-P explicitly in prequalification and qualification, ending a long-standing question from earlier editions.

Pulsed arc: one droplet per pulse time current transition current average current peak background one droplet detached per pulse tp tb The average stays below transition; each peak exceeds it. Real waveforms are programmed by the manufacturer.
Figure 4 — Pulsed-arc waveform. The average current stays below transition, but each peak exceeds it and detaches a droplet.

5.5 Controlled short circuit and inductance

Digital power sources monitor voltage and current in microseconds. In controlled short-circuit transfer, the source detects the instant the metal bridge is about to break and reduces current at that moment, eliminating the “explosion” that produces spatter; some variants also mechanically retract the wire to detach the droplet. Each manufacturer uses a trade name, but the principle is waveform control. The result is low heat input, good pipe roots and welding of thin, galvanized and aluminum sheet — on battery trays, it is common on thin covers, with pulsed transfer on thicker floors.

On conventional sources with inductance adjustment, increasing inductance reduces the rate of current rise during the short: the break is softer, with less spatter and better wetting. Too little inductance produces fine spatter and a convex bead; too much makes arc starting difficult.

ModePositionsHeat inputMain concern
Short circuitAllLowLack of fusion on thick sections; not prequalified in D1.1
GlobularFlat and horizontalMediumSpatter and irregular bead
SprayFlat and horizontal (steel)HighLarge pool; burn-through on thin sheet
PulsedAllLow to mediumHeat input calculated from instantaneous power
Controlled short circuitAllVery lowFusion on thick sections; qualify per code

6. Process parameters

  • Wire feed speed: sets current and deposition rate.
  • Voltage: mainly sets arc length and bead width. Too low, the arc “stubs”; too high, it causes undercut and porosity.
  • Travel speed: affects bead size, penetration and heat input.
  • Contact-tip-to-work distance (CTWD): changes current without anyone touching the source (see Figure 5).
  • Gun angles and gas flow: affect penetration, profile and shielding.
Contact-tip-to-work distance and electrode extension nozzle contact tip workpiece extension CTWD arc Increasing CTWD (fixed WFS): Electrical effect • more Joule heating of the wire • lower current and penetration Shielding effect • gas reaches the arc more diluted • higher porosity risk Keep the WPS distance. CTWD = electrode extension + arc length. Actual values come from the WPS.
Figure 5 — The electrode extension acts as a resistor in series with the arc: increasing it reduces current and penetration.

As a guide, short-circuit transfer uses shorter CTWD, in the order of 10 to 15 mm, and spray uses longer CTWD, in the order of 15 to 25 mm, always per the WPS.

Steel wire / modeWire feed speedApproximate currentApproximate voltage
1.0 mm — short circuit (M21)3 to 6 m/min90 to 150 A16 to 19 V
1.2 mm — short circuit (M21)3 to 5 m/min120 to 180 A17 to 20 V
1.2 mm — spray (M20/M21)8 to 14 m/min240 to 320 A27 to 32 V

Typical, indicative values only to show orders of magnitude; they do not replace the WPS or manufacturer data. AWS D1.1:2025 now links minimum currents to wire diameter for prequalified non-short-circuit GMAW — check the table in the current edition.

7. Worked calculations

7.1 Conventional load voltage (IEC 60974-1)

U₂ = 14 + 0.05 × I₂
U₂ in volts · I₂ in amperes · GMAW and flux-cored welding, used for testing and comparing power sources

Example: at 250 A, U₂ = 14 + 0.05 × 250 = 14 + 12.5 = 26.5 V. It is used for testing; the working voltage is the one in the WPS.

7.2 Deposition rate

Rate = vw × A × ρ × η
vw wire feed speed · A wire cross-section · ρ density · η deposition efficiency

Example: 1.2 mm steel wire at 8 m/min, ρ = 7.85 g/cm³ and η = 95%. Area: π × 0.6² ≈ 1.131 mm². Volume: 8000 mm/min × 1.131 mm² ≈ 9048 mm³/min = 9.05 cm³/min. Wire mass: 9.05 × 7.85 ≈ 71.0 g/min ≈ 4.26 kg/h. Deposited metal: 4.26 × 0.95 ≈ 4.05 kg/h. The deposition efficiency of GMAW with solid wire is typically above 90%, well above shielded metal arc welding.

7.3 Weld metal mass and arc time

A fillet weld with leg z = 6 mm has a theoretical cross-section z²/2 = 18 mm²; with 10% reinforcement, about 19.8 mm². Mass per meter: 19.8 mm² × 1000 mm × 7.85 × 10⁻³ g/mm³ ≈ 155 g/m. For 20 m: ≈ 3.11 kg. At 4.05 kg/h, arc time is 3.11 ÷ 4.05 ≈ 0.77 h. With a 40% operating factor (manual welding), total time is 0.77 ÷ 0.40 ≈ 1.9 h. In robotic cells the operating factor is much higher.

7.4 Heat input with controlled waveforms

Q = k × P ÷ v
Q in kJ/mm · k thermal efficiency (0.8 for GMAW in ISO/TR 17671-1) · P arc power in W · v travel speed in mm/s

In pulsed and controlled short-circuit transfer, the product of average voltage and average current does not represent the actual power. ISO/TR 18491 and ASME Section IX (QW-409.1) allow heat input to be calculated from instantaneous energy or power measured by the source or by a data acquisition system.

Example: a pulsed pass records 22 V and 180 A average (3.96 kW), but the measured average instantaneous power is 4.6 kW; travel speed 400 mm/min; k = 0.8. Using the product of averages: 0.8 × 3960 × 60 ÷ 400 000 ≈ 0.48 kJ/mm. Using instantaneous power: 0.8 × 4600 × 60 ÷ 400 000 ≈ 0.55 kJ/mm. The difference, about 16%, can make a procedure exceed the qualified heat input limit without anyone noticing.

7.5 Gas consumption and spool life

A cylinder with 10 m³ of mixture (example value; actual content depends on cylinder size and pressure) at 15 L/min supplies 10 000 ÷ 15 ≈ 667 min ≈ 11 h of arc-on time. A 15 kg spool of 1.2 mm wire holds 15 000 g ÷ 8.88 g/m ≈ 1690 m of wire (8.88 g/m = 1.131 mm² × 1000 mm × 7.85 × 10⁻³ g/mm³); at 8 m/min it lasts about 211 min ≈ 3.5 h of arc time.

7.6 Gun duty cycle

To estimate allowable current at another duty cycle, the usual thermal relation I₂ = I₁ × √(X₁ ÷ X₂) is used. A gun rated 300 A at 60% carries, at 100%, about 300 × √0.6 ≈ 232 A. It is an estimate; the manufacturer rating for the gas used is what counts.

8. Welding technique

With the gun tilted in the direction of travel (push), the arc acts on the still-cold metal ahead of the pool: the bead is wider and flatter, with less penetration and a better view of the joint. Tilted backwards (drag), penetration and reinforcement increase. On steel with solid wire both techniques are used, with a typical travel angle of 5° to 15°; with slag-forming tubular wires, the drag technique is most common; on aluminum, pushing is recommended to improve shielding and oxide removal. In vertical-down progression, the risk of lack of fusion on thick sections increases.

Weld starts and stops concentrate defects; power sources offer start ramps, crater fill and adjustable burnback time.

9. Procedures and qualification

The procedure specification follows ISO 15609-1 and is qualified by testing according to ISO 15614-1, or by ASME Section IX and AWS D1.1. Welders are qualified to ISO 9606-1, ASME IX or D1.1, and operators of mechanized and robotic equipment to ISO 14732. Pay special attention to:

  • Process and wire type: solid, flux-cored, metal-cored and self-shielded wires have different ISO 4063 numbers.
  • Transfer mode: under D1.1, short-circuit transfer requires qualification by testing; the same prequalified WPS cannot cover spray and short circuit.
  • Shielding gas: a change of group or composition may be an essential or supplementary variable, depending on the code.
  • Wire classification and heat input, when impact requirements apply.

D1.1:2025 also reorganized prequalification into process-specific tables and made the preheat and interpass temperature fields mandatory (“shall”) in WPSs.

Block 2 summary

Short-circuit, globular, spray and pulsed transfer have distinct fields of application, and controlled short-circuit transfer extended the process to thin sheet and low-heat roots. CTWD is a hidden electrical variable. Transfer mode, gas and wire are qualification variables.

Original, conceptual diagrams. Transition currents, parameter ranges and qualification rules must be confirmed in current standards and manufacturer data sheets.

EXCELLENCE INDUSTRIAL TECH • ARTICLE IT-003 • BLOCK 3 OF 3

Wire Feeding, Quality, Safety, Current Technology and Assessment

Feeding failures, imperfections and troubleshooting, inspection, safety and fume, robotics, artificial intelligence, tandem, MIG brazing, WAAM, case study and a 30-question test.

10. Wire feeding and gun maintenance

Many GMAW problems are not in the arc but along the path the wire travels from the spool to the contact tip. Friction or slack becomes erratic wire speed, erratic current and an unstable arc, even with correct parameters.

Wire path and failure points Spool brake too tight rusty wire crossed wraps Drive rolls wrong groove excess pressure worn groove misalignment Liner dirty or kinked too long wrong type (steel × PTFE) Gun blocked diffuser nozzle with spatter gas leak Tip oval bore wrong size loose thread stuck spatter Friction or slack at any stage becomes erratic feed, erratic current and an unstable arc.
Figure 6 — Wire path. Preventive maintenance of drive rolls, liner, diffuser and tip eliminates most arc problems blamed on the power source.
ProblemFrequent causesCorrection
Bird-nesting at the drive rollsExcess pressure, blocked or long liner, clogged tip, wrong rollsAdjust pressure, clean or replace liner, replace tip, use correct rolls
Wire fusing to the tip (burnback)Erratic feeding, CTWD too short, burnback time poorly setCorrect feeding, keep CTWD, adjust burnback
Unstable arc and fluctuating currentWorn or loose tip, poor work return cableReplace tip, tighten connections, clamp close to the joint
Intermittent porositySpatter in nozzle, blocked diffuser, leak in gun or hoseClean nozzle and diffuser, leak test, replace hose

11. Typical imperfections and troubleshooting

ISO 6520-1 classifies imperfections by reference numbers (for example, 2011 for gas pore, 401 for lack of fusion, 5011 for continuous undercut, 510 for burn-through and 602 for spatter), and ISO 5817 — 2023 edition — or the design code sets acceptance limits in quality levels B, C and D.

SymptomProbable causeCheckCorrection
Scattered or surface poresPoor shielding: drafts, flow, leak, dirty nozzleFlowmeter at the nozzle, leak test, diffuser inspectionScreen, WPS flow, cleaning, hose replacement
Aligned pores on galvanized jointsTrapped zinc vaporCoating thickness, joint gapVenting gap, local removal, pulsed or controlled short circuit
Sidewall lack of fusionShort circuit on thick plate, high travel speed, wrong angleMacro-etch, ultrasonic testing, mode reviewSpray or pulsed, WPS angle and speed
Excessive spatterVoltage too low for wire speed, CO₂, inductance, worn tipParameter record, tip conditionAdjust voltage and inductance, Ar+CO₂ mixture, replace tip
Burn-throughHigh current on thin sheet, excessive root openingThickness, opening, modeShort circuit or pulsed, adjust gap, backing bar
Silicate islandsWire deoxidizers (Mn, Si)Dark glassy deposits on the beadRemove before painting or coating
Porosity troubleshooting: order of checks 1. Environment drafts, doors, fans 2. Gas flow, hose, fittings 3. Gun clean nozzle and diffuser 4. Workpiece oil, paint, zinc, moisture 5. Technique WPS CTWD and angle 6. Parameters only then review if all OK Raising the flow rate without finding the cause usually worsens shielding. Teaching sequence; record each check and its result.
Figure 7 — Porosity troubleshooting. Order matters: starting with environment and shielding avoids changing parameters unnecessarily.

12. Inspection

Visual testing follows ISO 17637, before (preparation, gas, wire, parameters) and after welding (dimensions, undercut, pores, craters). Lack of fusion from short-circuit transfer may not show on the surface; macro-etch, ultrasonic and radiographic testing, per the code, detect it. In series production, per-weld data monitoring identifies deviations before they become rejected batches.

13. GMAW safety

  • Radiation: spray and pulsed arcs with argon emit intense ultraviolet radiation; the filter must suit the current (ISO 16321 series, ANSI Z87.1); clothing per ISO 11611.
  • Fume: IARC classifies welding fume as carcinogenic to humans (Group 1). Tubular wires generate more fume than solid wires; manganese (carbon steel) and hexavalent chromium (stainless) are the main concerns. ACGIH recommends a TLV of 0.02 mg/m³ for respirable manganese, far below the OSHA legal limit. Source capture (arms, hoods and fume-extraction guns; ISO 21904 series) is the first measure.
  • Gases: cylinders upright, secured, with valve caps and suitable regulators. Argon, helium and CO₂ displace oxygen in confined spaces.
  • Ozone: ultraviolet radiation forms ozone, especially on aluminum and stainless steel.
  • Robots: cells must have guards, interlocks and energy isolation for maintenance, including collaborative applications.
Standards and regulations: ANSI Z49.1 and OSHA 29 CFR 1910 Subpart Q (1910.252 to 1910.254) in the United States; IEC 60974-1 for power sources; ISO 10218-1 and ISO 10218-2, revised in 2025, for robots and robot applications — the new edition incorporates the requirements of former ISO/TS 15066 for collaborative applications and adds cybersecurity requirements. In Brazil, NR-12 (comparable to ISO 12100 and ISO 10218), NR-6 (PPE), NR-33 (confined spaces, comparable to OSHA 29 CFR 1910.146) and, in shipbuilding, NR-34 set applicable requirements.

Regulatory trend: Australia lowered its welding fume exposure limit from 5 to 1 mg/m³ in 2024 and adopts a new list of limits on 1 December 2026; the European Commission proposed in July 2025 to include welding fume in the carcinogens directive; and NIOSH reported in 2026 shipyard welders exposed to manganese above recommended values.

14. Old × current × next technology

AspectTraditional practiceCurrent practice (2024–2026)Trend
Power sourceTapped transformerSynergic inverter, pulsed and controlled short circuitWaveforms updated by software
ParametersWritten by handRecorded per weldAutomatic real-time correction
RobotPoint-to-point teachingSeam tracking; cobots in smaller batchesAutomatic programming from the 3D model
QualityFinal visual inspectionData monitoring and visionAI reading the weld pool image
FumeGeneral ventilationSource captureLower limits and continuous measurement

14.1 Robotics, seam tracking and artificial intelligence

Robotic repeatability depends on accurate fixturing, TCP calibration, automatic nozzle cleaning, seam tracking and per-weld monitoring. In 2026, the frontier is adaptive control: research and manufacturer projects — such as the European AITOOLS1 consortium, focused on lot-size-one robotic welding, and EPRI adaptive systems for GMAW and GTAW — combine machine vision, synchronized data and machine learning to correct path and parameters in response to fit-up variation. AI-guided heavy-duty robots already make root passes on offshore structures.

14.2 Tandem GMAW and hybrid laser-GMAW

In the tandem process, two electrically insulated wires, each with its own synchronized power source, feed the same pool, with much higher deposition on beams, railcars and wind towers. In hybrid laser-GMAW, the laser penetrates and the arc tolerates gaps — a combination used on battery trays and in shipbuilding.

14.3 MIG brazing

In MIG brazing, used in the automotive industry on galvanized and high-strength steels, the filler metal is a copper alloy (for example, CuSi3 or CuAl8) that melts below the melting temperature of steel. The base metal does not melt, most of the zinc is preserved and distortion is lower; inert gas is used with pulsed or controlled short-circuit transfer.

14.4 Wire arc additive manufacturing (WAAM)

Wire arc additive manufacturing uses GMAW, usually with controlled short-circuit or pulsed transfer, to build large parts layer by layer from a digital model. In ISO/ASTM 52900 terminology, it falls under directed energy deposition; AWS D20.1 covers fabrication by additive manufacturing. WAAM requires strict control of interpass temperature, heat input and path; parts require final machining.

14.5 What comes next

Trends point to cells that program themselves from the 3D model and vision, digital welding records as quality evidence along the supply chain, and digital twins that simulate distortion before the first part. An amendment to ISO 4063:2023 is under development. None of this replaces the fundamentals.

15. Case study — porosity after a change of location

A team welding brackets with GMAW (ER70S-6, M21, 1.2 mm) was moved to an open shed near a gate. The welds began to show porosity. The first reaction was to raise the flow from 15 to 30 L/min and increase the voltage.

Analysis: the higher flow created turbulence and worsened shielding. Following Figure 7, the investigation found three causes: draft from the gate, spatter built up in the nozzle and a small crack in the gas hose near the feeder.

Correction: wind screen, hose replacement, cleaning of nozzle and diffuser, flow back to the WPS range and voltage back to the original value. The porosity disappeared with no procedure change.

Technical lesson: before changing parameters, check environment, gas shielding, leaks and gun.

16. GMAW operator checklist

  • ☐ Check wire (classification and diameter), gas (ISO 14175 designation) and transfer mode in the WPS.
  • ☐ Check drive rolls, liner, contact tip, diffuser and nozzle are compatible and clean.
  • ☐ Set flow at the nozzle outlet and leak-test.
  • ☐ Protect the workstation from drafts.
  • ☐ Keep CTWD constant and per the WPS.
  • ☐ Confirm heat input from the energy shown by the source, when a limit applies.
  • ☐ Remove silicate islands before painting or coating.
  • ☐ Switch on fume extraction and wear full PPE.
  • ☐ Record parameters, wire batch and inspection result.

17. Frequently asked questions

Can I use M21 instead of CO₂ with the same flux-cored wire? Only if the wire is classified for both gases (M and C suffixes in AWS, M21 and C1 in ISO) and the WPS allows it. The gas changes the deposit chemistry and mechanical properties.

Why does my GMAW spatter so much with CO₂? CO₂ prevents axial spray transfer and favors large, repelled droplets. Voltage and inductance help; an Ar-CO₂ mixture or controlled short circuit works better.

Can I still use wires classified to AWS A5.36? The product still exists, but the specification was withdrawn. For work to D1.1:2025, the WPS must reference the equivalent classification in A5.18, A5.20, A5.28 or A5.29, per the manufacturer certificate.

18. Technical test — 30 multiple-choice questions

Choose one answer per question and check the commented answer key in the next section.

Question 1 — With a constant-voltage source, the welder pulls the gun away and the arc becomes longer. What happens immediately?

A) The source raises current to keep arc power constant and quickly restore the arc length.
B) Current does not change, since wire speed is fixed; only voltage rises.
C) Current drops, the wire melts more slowly and advances until the arc recovers.
D) The feeder slows down until voltage returns to the set value.

Question 2 — Technician A says that, in ISO 4063, 136 is MAG with flux-cored wire and 114 is self-shielded flux-cored wire. Technician B says 138 is MIG with inert gas and solid wire. Who is right?

A) Technician A only.
B) Technician B only.
C) Both.
D) Neither.

Question 3 — A cylinder is labeled ISO 14175 – M20 – ArC – 8. Which conclusion is correct?

A) Argon with 20% CO₂, for spray on steel.
B) Argon with 8% O₂, a strongly oxidizing mixture.
C) Inert gas with 8% helium, for thick aluminum.
D) Argon with 8% CO₂, within subgroup M20 (over 5% up to 15% CO₂).

Question 4 — In GMAW of steel with solid wire, which polarity is normally specified and why?

A) DCEN, which concentrates heat in the wire and raises deposition without losing stability.
B) DCEP, which gives a stable arc, regular transfer and good penetration.
C) Alternating current, which reduces arc blow and balances the heat.
D) DCEN for carbon steel and DCEP only for aluminum, because of the oxide.

Question 5 — Why is axial spray not obtained with pure CO₂, even at high currents?

A) CO₂ ionizes more easily than argon, which cools the column and reduces effective current.
B) Forces under the droplet push it upward, forming large, repelled droplets.
C) CO₂ reacts with the wire copper and forms slag that holds the droplet.
D) The constant-voltage source limits current when the gas is active.

Question 6 — When changing from 1.0 mm steel wire to 1.2 mm aluminum wire on the same feeder, what must change?

A) U-groove rolls, PTFE or graphite liner, suitable tip and lower pressure.
B) Only the contact tip, since a coiled steel liner suits any wire larger than the previous one.
C) Knurled rolls for traction and a steel liner for less friction.
D) Only the gas, from M21 to I1, keeping V-groove rolls and steel liner.

Question 7 — With wire feed speed and voltage unchanged, CTWD goes from 15 to 25 mm. Expected effect?

A) Current rises, because the longer wire carries more current.
B) Penetration increases, because the arc becomes longer, wider and hotter on the base metal.
C) Current and penetration drop, due to Joule preheating of the wire.
D) Nothing changes, as the source compensates any extension change.

Question 8 — Technician A says raising flow from 15 to 35 L/min always improves shielding in wind. Technician B says M21 protects the pool even in drafts because it is denser than air. Who is right?

A) Technician A only.
B) Technician B only.
C) Both.
D) Neither.

Question 9 — Dark glassy flakes appear on GMAW beads made with ER70S-6. Origin and action?

A) Silicates from wire deoxidizers (Mn, Si); remove before painting or coating.
B) Copper inclusions from a worn contact tip; reject and completely reweld the joint.
C) Flux slag: the wire in use is tubular, not solid.
D) Copper oxide from the wire; change to uncoated wire.

Question 10 — In AWS A5.18, what does ER70S-6 indicate?

A) Covered electrode with 70 ksi yield strength, all positions, coating type 6.
B) Solid wire with 70% Mn and Si in range 6, for CO₂ only.
C) Solid electrode or rod, 70 ksi minimum tensile, chemistry type 6.
D) Tubular wire of 70 ksi, classified for six positions.

Question 11 — 1.0 mm steel wire at 10 m/min, density 7.85 g/cm³ and 92% efficiency. Approximate deposition rate?

A) 3.70 kg/h.
B) 3.40 kg/h.
C) 13.6 kg/h.
D) 0.06 kg/h.

Question 12 — Pulsed pass: 23 V and 200 A average, average instantaneous power 5.2 kW, 500 mm/min, k = 0.8. Heat input by the instantaneous power method?

A) 0.44 kJ/mm.
B) 0.62 kJ/mm.
C) 0.55 kJ/mm.
D) 0.50 kJ/mm.

Question 13 — Short circuit with CO₂: convex bead, much fine spatter, poor wetting. The source has inductance adjustment. What tends to help?

A) Increase inductance, softening the current rise during the short.
B) Reduce inductance, so current rises faster and breaks the bridge with more energy.
C) Set inductance to zero and raise wire speed by 30%.
D) Keep inductance and switch polarity to DCEN.

Question 14 — Technician A says that, in AWS D1.1, short-circuit transfer (GMAW-S) is not prequalified and requires qualification by testing. Technician B says its typical risk on thick plate is lack of fusion, often invisible on the surface. Who is right?

A) Technician A only.
B) Technician B only.
C) Both.
D) Neither.

Question 15 — Manufacturer table: spray from about 220 A for 1.1 mm steel wire with Ar + 2% O₂. The operator welds at 190 A, same mixture, high voltage, and sees large droplets and spatter. Diagnosis?

A) Cylinder contaminated with more than 20% CO₂.
B) Current below transition: globular transfer.
C) Excessive inductance delaying current in the short.
D) Polarity reversed to DCEN, enlarging the droplet.

Question 16 — Correct sequence to investigate porosity that suddenly appeared at a manual GMAW station:

A) Raise voltage, raise flow, change wire, check drafts.
B) Change gas, change wire, reduce speed, check nozzle.
C) Raise flow, clean nozzle, check drafts, review WPS.
D) Environment and leaks, nozzle and diffuser, workpiece and CTWD, and only then parameters.

Question 17 — All are probable causes of bird-nesting at the drive rolls, EXCEPT:

A) Gas flow below the WPS range.
B) Clogged tip or tip bore smaller than the wire.
C) Long, kinked or dirty liner.
D) Excess roll pressure deforming the wire.

Question 18 — Technician A says AWS A5.36 is the current specification that replaced A5.20 and A5.18 for flux-cored and metal-cored wires. Technician B says that, in AWS A5.18, carbon steel metal-cored wires may be classified as E70C-6M. Who is right?

A) Technician A only.
B) Technician B only.
C) Both.
D) Neither.

Question 19 — A gun is rated 300 A at 60% duty cycle. Using I₂ = I₁ × √(X₁ ÷ X₂), what is the estimated current at 100%?

A) 180 A.
B) 300 A.
C) About 232 A.
D) About 387 A.

Question 20 — A wire is marked ISO 17632-A: T 46 4 P M21 1 H5. Which reading is correct?

A) Re ≥ 460 MPa, 47 J at −40 °C, fast-freezing rutile core, M21 gas, all positions, H ≤ 5 mL/100 g.
B) Rm ≥ 460 MPa, 27 J at −40 °C, metal core, CO₂, flat position.
C) Re of 46 ksi, impact at −4 °C, basic core, one position.
D) Solid wire of 460 MPa with 4% nickel, tested with M21.

Question 21 — What principle is common to controlled short-circuit processes sold under different trade names?

A) High-frequency AC to detach the droplet without a short.
B) Keep inductance fixed at maximum, with no reading of the arc electrical signals.
C) A core flux that stabilizes the metal bridge.
D) Detect the bridge rupture and cut current at that instant.

Question 22 — Cell with per-weld monitoring: average current falls during the shift, with constant wire speed and voltage, and spatter increases. Most likely cause?

A) Variation of M21 between cylinders of the same batch.
B) Worn or spatter-loaded contact tip, changing the contact point and effective extension.
C) Return cable heating that raises open-circuit voltage.
D) TCP error increasing programmed travel speed.

Question 23 — In MIG brazing of galvanized steel in the automotive industry, it is correct to state:

A) The steel partly melts and alloys with CuSi3, becoming stronger than steel.
B) Pure CO₂ is used to penetrate and burn off all zinc before deposition.
C) The copper alloy melts below the steel and preserves much of the zinc.
D) It requires preheating to about 600 °C to evaporate the zinc.

Question 24 — In WAAM, which variable is most critical to avoid heat build-up, distortion and geometry variation between layers?

A) Interpass temperature, via dwell times and path strategy.
B) Spool diameter, which limits wire speed per layer.
C) Gas flow raised to about 40 L/min to cool the part.
D) Gun cable length, which changes inductance and layer height.

Question 25 — What characterizes tandem GMAW?

A) One wire fed by two synchronized feeders.
B) Two wires at the same electrical potential, connected to one source, to double the arc current.
C) Cold wire added to the pool of a GTAW arc.
D) Two insulated wires, with their own synchronized sources, in the same pool.

Question 26 — After installing fume-extraction guns, pores appear in the welds. Most likely explanation and correction?

A) Extraction raises current; reduce wire speed.
B) Suction removes the gas; adjust suction flow and nozzle per the manufacturer.
C) Captured fume contaminates the wire; use self-shielded wire.
D) Extraction creates inductance in the cable; reduce source inductance.

Question 27 — Technician A says that, with waveform-controlled sources, the product of average voltage and current may underestimate arc power. Technician B says that, therefore, ASME Section IX allows heat input to be calculated from instantaneous energy or power. Who is right?

A) Technician A only.
B) Technician B only.
C) Both.
D) Neither.

Question 28 — On a synergic source set to “steel, 1.2 mm, M21”, the welder increases wire speed. What does the source do?

A) Adjusts voltage (and, in pulsed mode, the pulse) per the wire and gas curve.
B) Keeps voltage constant and lowers current to preserve the programmed heat input.
C) Switches by itself to controlled short circuit.
D) Adjusts gas flow in proportion to current.

Question 29 — To change the tip in a robotic GMAW cell, which procedure meets ISO 10218-2, ISO 12100 and, in Brazil, NR-12?

A) Slow the robot to 10% and enter with the program running.
B) Pause from the HMI and enter, since the arc is off.
C) Switch off only the power source, keeping the robot energized.
D) Lock out and tag out the energies, verify their absence and only then enter.

Question 30 — For horizontal fillets on beams, a company replaces ER70S-6 with E70C-6M metal-cored wire of the same diameter. Which gain is consistent?

A) No more fume or shielding gas.
B) Higher deposition and better sidewall fusion, with little slag and keeping the gas.
C) Use of DCEN with any wire, with no effect on arc stability or on the weld penetration depth.
D) No requalification, since the ISO 4063 number is the same.

19. Commented answer key

1 — C. On a flat curve, a longer arc sharply reduces current and the wire advances (self-regulation). A describes a constant-power source.

2 — A. 136 is MAG with flux-cored wire and 114 is self-shielded; 138 is MAG with metal-cored wire — MIG with solid wire is 131.

3 — D. M20 covers Ar with over 5% up to 15% CO₂; “ArC – 8” means 8% CO₂. A confuses subgroup with content.

4 — B. DCEP gives a stable arc and good penetration; DCEN (A) applies only to some self-shielded wires.

5 — B. With CO₂, forces under the droplet repel it and transfer becomes globular. A attributes the effect to arc cooling, which does not occur.

6 — A. Aluminum needs U-groove rolls, a low-friction liner, a suitable tip and less pressure; knurled rolls (C) damage the wire.

7 — C. The longer extension is Joule-preheated and needs less current. D ignores that the source holds voltage, not current.

8 — D. Excessive flow creates turbulence and draws in air, and no mixture resists wind: both are wrong.

9 — A. They are Mn and Si silicates from the deoxidizers; they do not reject the weld (B) but impair painting.

10 — C. ER = electrode or rod, 70 ksi tensile, S = solid, 6 = chemistry. A confuses it with a covered electrode and with yield.

11 — B. π × 0.5² × 10 000 × 7.85 × 10⁻³ × 60 ÷ 1000 ≈ 3.70 kg/h; × 0.92 ≈ 3.40 kg/h. A omits efficiency; C uses diameter as radius.

12 — D. 0.8 × 5200 × 60 ÷ 500 000 ≈ 0.50 kJ/mm. A uses the product of averages (4.6 kW); B omits k.

13 — A. More inductance softens the short, reduces spatter and wets the bead; reducing it (B) increases fine spatter.

14 — C. D1.1 excludes GMAW-S from prequalification precisely because of the lack-of-fusion risk: both are right.

15 — B. Below transition, transfer is globular. A has no evidence; the table already explains the symptom.

16 — D. First environment and shielding, then gun, workpiece and technique; parameters last. C starts by raising flow.

17 — A. Gas flow does not affect wire traction; B, C and D cause jamming or friction.

18 — B. A5.36 was withdrawn in 2023; carbon steel metal-cored wires are classified in A5.18 as E70C-6M. Only B is right.

19 — C. 300 × √0.6 ≈ 232 A. A multiplies by the fraction; D inverts the relation.

20 — A. T, 46 (Re ≥ 460 MPa), 4 (47 J at −40 °C), P (fast-freezing rutile), M21, 1 (all positions), H5. B mixes systems A and B.

21 — D. The control senses the short and cuts current at rupture. B describes inductance, with no active control.

22 — B. A worn tip changes the contact point and effective extension: current drops. A is unlikely within the same certified batch.

23 — C. The copper alloy melts below the steel, which does not melt. A describes fusion welding, not brazing.

24 — A. Interpass temperature and path control heat build-up; high flow (C) only creates turbulence.

25 — D. Tandem uses two insulated wires with synchronized sources; B describes single-potential twin wire.

26 — B. Excessive suction removes the shielding; the manufacturer setting (ISO 21904 series) solves it. A has no physical link.

27 — C. Averages underestimate power in controlled waveforms; ASME IX (QW-409.1) and ISO/TR 18491 accept instantaneous energy.

28 — A. Synergy adjusts voltage and pulse along the curve. B describes heat-input control that synergy does not perform.

29 — D. Intervention requires lockout and verification of zero energy; a software pause (B) can be reversed.

30 — B. Metal-cored wire keeps the gas, deposits more and fuses sidewalls better; D is false: 135 and 138 are different numbers.

Performance interpretation

  • 27 to 30 correct: excellent command of the process and current technologies.
  • 22 to 26 correct: good command, with specific points to review.
  • 16 to 21 correct: review the blocks related to the missed questions.
  • 0 to 15 correct: theoretical reinforcement and supervised practice are recommended.

20. Technical references

  • ISO 4063:2023: nomenclature and reference numbers of processes.
  • ISO 14175 and AWS A5.32M/A5.32:2021: shielding gases and mixtures.
  • AWS A5.18/A5.18M:2023, AWS A5.20/A5.20M:2021, AWS A5.28, A5.29, A5.9, A5.10 and A5.22: solid, flux-cored and metal-cored wires; AWS A5.36/A5.36M:2016 (withdrawn in 2023).
  • ISO 14341, ISO 17632, ISO 16834, ISO 17634, ISO 18276, ISO 21952, ISO 14343, ISO 17633 and ISO 18273: consumable classification.
  • IEC 60974-1, IEC 60974-7 and IEC 60974-14: power sources, guns and calibration.
  • ISO/TR 17671-1 and ISO/TR 18491: welding recommendations and energy measurement for waveforms.
  • ISO 15609-1, ISO 15614-1, ISO 9606-1, ISO 14732, ASME Section IX, AWS D1.1/D1.1M:2025 and AWS D1.3: procedures and qualification.
  • ISO 6520-1, ISO 5817:2023 and ISO 17637: imperfections, quality levels and visual testing.
  • ANSI Z49.1, OSHA 29 CFR 1910 Subpart Q, ISO 11611, ISO 16321 series, ISO 21904 series, ISO 10218-1:2025 and ISO 10218-2:2025: safety.
  • ISO/ASTM 52900 and AWS D20.1: additive manufacturing.
  • Brazil: NR-6, NR-12, NR-33 and NR-34, compared with international equivalents in the text.
  • Teaching base: ESAB MIG/MAG welding handbook, Brazilian edition (2005), paraphrased and updated.

Note: standards must be consulted in their current editions. National equivalents may exist in each country.

21. Conclusion

GMAW looks simple, but every bead depends on the right gas and wire by classification, the right transfer mode, constant CTWD and friction-free feeding. Pulsed and controlled short-circuit transfer, data recording and AI-based adaptive control have extended the process, while D1.1:2025, ISO 10218:2025 and the pressure on fume have changed the rules. Those who master the fundamentals take advantage of technology; those who do not automate their own defects.

EXCELLENCE INDUSTRIAL TECH

After studying the three blocks, take the Gas Metal Arc and Flux-Cored Arc Welding test in the Excellence Industrial Tech app and track your performance in the ranking.

Technical note: educational content. Values and examples are for teaching; procedures, parameters and acceptance criteria must follow the standards, the WPS and the manufacturers’ documentation.